真空蒸馏-分级冷凝法提纯锑

谈仁杰 ,  田庆华 ,  辛云涛 ,  许志鹏

有色金属(冶炼部分) ›› 2026, Vol. 0 ›› Issue (11) : 2323 -2336.

PDF (17314KB)
有色金属(冶炼部分) ›› 2026, Vol. 0 ›› Issue (11) : 2323 -2336. DOI: 10.20237/j.issn.1007-7545.2026.11.005

真空蒸馏-分级冷凝法提纯锑

作者信息 +

Antimony Purification by Vacuum Distillation and Fractional Condensation

Author information +
文章历史 +
PDF (17729K)

摘要

为降低工业锑中As、Pb 和Bi 等杂质含量,采用真空蒸馏-分级冷凝法开展提纯试验,考察蒸馏温度和保温时间对锑挥发、产品纯度、直收率及杂质分布的影响,并结合饱和蒸气压、蒸气碰撞和均质形核计算分析组元分离行为。结果表明:在973~1 073 K 的范围内,Sb 饱和蒸气压随温度升高增大,促进锑由熔体向冷凝区迁移;降低冷凝温度或提高锑分压均增大过饱和度,并降低临界核半径和形核势垒。保温6 h 时,1# 冷凝壁产品纯度和直收率在1 033 K 达到最高值,继续升温后均下降。1 033 K 下,延长保温时间可提高锑回收量,12 h 时直收率约为82%。综合产品质量和试验周期,在炉内总压100 Pa、蒸馏温度1 033 K、第一冷凝区设定温度773 K、保温6 h 的条件下,1# 冷凝壁获得纯度99.99% 的锑产品,As、Pb 和Bi 含量分别为36.91、8.19、4.12 mg/kg。Pb主要向残留物分配,As在后续冷凝区域富集;将各冷凝区的冷凝物分别收集,可以实现锑与主要杂质的分离。

Abstract

The separation of arsenic, lead, and bismuth from industrial antimony was investigated to determine suitable distillation conditions and product collection locations. Vacuum distillation was combined with fractional condensation, and the effects of distillation temperature and holding time on volatilization, product purity, direct yield, and impurity distribution were examined. Saturation vapor pressure, vapor collision frequency, and homogeneous nucleation calculations were used to interpret the separation behavior of antimony and its major impurities during evaporation and condensation. Industrial cathode antimony was treated in a vertical vacuum furnace equipped with a custom high-purity graphite crucible and staged graphite condensers. The feed contained 240.5, 410.0, and 30.5 mg/kg of As, Pb, and Bi, respectively. The evaporation zone and first condensation zone were separately temperature-controlled. Each experiment used a 200 g charge, a total furnace pressure of 100 Pa constrained by the available vacuum equipment, and a first-condensation-zone setpoint of 773 K, corrected using a temperature calibration ring. The temperatures at individual collection surfaces were not measured separately. The charge was heated to the target evaporation temperature over 2 h. Temperature experiments were conducted at 973, 993, 1 013, 1 033, 1 053, and 1 073 K for 6 h, whereas holding times of 4, 6, 8, 10, and 12 h were examined at 1 033 K. After cooling, the residue and deposits on each condenser wall and cover were collected and weighed separately. Impurity contents were measured by inductively coupled plasma mass spectrometry (ICP-MS). The deposit on the first condenser wall was designated as the target product, and its direct yield was calculated as the product mass divided by the initial feed mass. The results show that the calculated saturation vapor pressure of Sb increases from 65.26 Pa to 273.7 Pa between 973 K and 1 073 K, corresponding to a 4.19-fold increase. Pb and Bi show lower intrinsic volatility than Sb, whereas As shows a stronger tendency to enter the vapor phase. These differences support the retention of Pb and Bi at the evaporation end and the subsequent separation of As through staged condensation. Collision calculations use reference component partial pressures of 1, 10, and 20 Pa. At a fixed partial pressure, the calculated collision frequency decreases gradually with increasing temperature; at a fixed temperature, it increases proportionally with partial pressure. Cooling and increasing the Sb partial pressure both increase the calculated supersaturation. Component reference pressures used in the condensation calculations are distinguished from the total furnace pressure relevant to evaporation and vapor transport. Classical homogeneous nucleation calculations compare liquid and solid nuclei over 723–823 K. The liquid pathway represents supercooled liquid nuclei because this temperature range is below the bulk melting point of Sb. At an Sb partial pressure of 10 Pa, cooling from 823 K to 723 K reduces the liquid critical radius from 2.17 nm to 0.667 nm and the nucleation barrier from 647 kB T to 70.2 kB T, where kB denotes the Boltzmann constant and T denoted thermodynamic temperature. At 773 K and 10 Pa, the liquid and solid critical radii are 1.02 and 1.34 nm, and the corresponding barriers are 153 and 423 kBT. The liquid pathway has a lower barrier under the adopted interfacial-energy parameters. This comparison describes the relative tendencies of the two modeled pathways; it does not establish the actual phase of the initial nuclei. In the temperature series, volatilization increases from 4.64% at 973 K to 34.26% at 1 033 K and remains above 34% at 1 053–1 073 K. At 1 033 K, the first condenser-wall product reaches a purity of 99.9924% and a mass yield of 28.61%. Further heating reduces the target product yield to about 26% and its purity to approximately 99.962% at 1 073 K. The additional evaporation at higher temperatures thus does not translate into a corresponding increase in collected high-purity product. At 1 033 K, extending the holding time increases the volatilized fraction, which exceeds 90% after 12 h. Product direct yield increases overall and reaches 82.33% at 12 h, the highest value in the time series. Product purity varies with time and remains relatively high at both 6 and 12 h. A holding time of 6 h is selected for the regional composition analysis after considering product purity and processing duration. This condition provides high-purity antimony within a shorter holding period, whereas 12 h favores greater recovery per batch. At 1 033 K with a first-condensation-zone setpoint of 773 K and a holding time of 6 h, the first condenser-wall product reaches 99.9924% purity at a direct yield of 28.61%. Its As, Pb, and Bi contents are 36.91, 8.19, and 4.12 mg/kg, respectively. The Pb content of the residue is approximately 600 mg/kg, compared with 410.0 mg/kg in the feed. As contents reach approximately 5 800 mg/kg on the second condenser wall and 2 200 mg/kg on its cover. The first condenser cover also contains more As than the first condenser wall. These distributions demonstrate the need to collect deposits from different regions and surfaces separately. The combined experimental and calculated results support a separation mechanism involving selective evaporation followed by spatial separation during condensation. Preferential retention at the evaporation end restricts Pb and Bi transfer, while downstream enrichment of As reduces its incorporation into the target Sb deposit. Independent collection from the first condenser wall enables the preparation of antimony with a purity above 99.99%. Suitable evaporation intensity and separate collection of As-rich condensates are the principal operating requirements identified for this process. The limited degree of evaporation at 100 Pa contributes to the low 6 h product yield. Improving the vacuum system to lower the absolute pressure is expected to enhance evaporation and increase product yield when sufficient selective condensation is maintained.

关键词

真空蒸馏 / 分级冷凝 / 锑 / 提纯 / 杂质分布

Key words

vacuum distillation / fractional condensation / antimony / purification / impurity distribution

引用本文

引用格式 ▾
谈仁杰,田庆华,辛云涛,许志鹏. 真空蒸馏-分级冷凝法提纯锑[J]. 有色金属(冶炼部分), 2026, 0(11): 2323-2336 DOI:10.20237/j.issn.1007-7545.2026.11.005

登录浏览全文

4963

注册一个新账户 忘记密码

参考文献

[1]

王成彦, 邵爽, 马保中, 等 . 中国锑铋冶金现状及进展[J]. 有色金属(冶炼部分), 2019(8): 11-17.

[2]

Wang Chengyan, Shao Shuang, Ma Baozhong, et al. Status and development of antimony and bismuth metallurgy technologies in China[J]. Nonferrous Metals (Extractive Metallurgy), 2019(8): 11-17.

[3]

唐谟堂, 唐朝波, 杨建广, 等 . 双碳战略下中国锑产业发展趋势[J]. 有色金属(冶炼部分), 2024(11): 110-116.

[4]

Tang Motang, Tang Chaobo, Yang Jianguang, et al. Development trend of antimony industry in China under dual carbon strategy[J]. Nonferrous Metals (Extractive Metallurgy), 2024(11): 110-116.

[5]

Li Zongbo, Feng Yan, Wen Yufeng, et al. Preparation technology research progress of high-purity antimony[J]. Transactions of Nonferrous Metals Society of China, 2025, 35(2): 579-601.

[6]

谈仁杰, 田庆华, 辛云涛, 等 . 高纯锑的制备技术及其应用[J]. 有色金属(冶炼部分), 2026(9): 1813-1837.

[7]

Tan Renjie, Tian Qinghua, Xin Yuntao, et al. Preparation technologies and application progress of high-purity antimony[J]. Nonferrous Metals (Extractive Metallurgy), 2026(9): 1813-1837.

[8]

Kong Junfeng, Cao Huazhen, Qian Weilun, et al. Deep removal of trace arsenic from acidic SbCl3 solution by in-situ galvanically coupled Cu2Sb/Cu particles [J]. Journal of Hazardous Materials, 2024, 467: 133659. DOI: 10.1016/j.jhazmat.2024.133659.

[9]

Zhang Xiaoxin, Friedrich S, Friedrich B . Separation behavior of arsenic and lead from antimony during vacuum distillation and zone refining[J]. Journal of Materials Research and Technology, 2020, 9(3): 4386-4398.

[10]

Li Yaxing, Li Zongbo, Wang Richu, et al. The separation behavior of impurity in antimony during vacuum distillation[J]. Vacuum, 2023, 211: 111669. DOI: 10.1016/j.vacuum.2022.111669.

[11]

Zheng Lin, Zhang Lei, Nan Changbin, et al. A novel model of bismuth and lead impurities removal behavior in purification of antimony metal by vacuum distillation[J]. Vacuum, 2023, 211: 111910. DOI: 10.1016/j.vacuum.2023.111910.

[12]

Xu Changyi, Zeng Yuanlin, Wang Zhaoyi, et al. The volatilization law of standard impurity elements in 3N antimony during vacuum distillation and preparing antimony with 4N8 content[J]. Separation and Purification Technology, 2025, 355: 129675. DOI: 10.1016/j.seppur.2024.129675.

[13]

程越伟, 张环, 车玉思, 等 . 含砷锑物料真空挥发-定向冷凝工艺研究[J]. 有色金属(冶炼部分), 2025(8): 63-72.

[14]

Cheng Yuewei, Zhang Huan, Che Yusi, et al. Research on vacuum evaporation-directional condensation process of materials containing arsenic and antimony[J]. Nonferrous Metals (Extractive Metallurgy), 2025(8): 63-72.

[15]

Zhang Lei, Li Jiaxuan, Zhou Yi, et al. Preparation of multiplex purity antimony metal via vacuum distillation combined with selective condensation[J]. Materialia, 2025, 44: 102574. DOI: 10.1016/j.mtla.2025.102574.

[16]

Chen Liangliang, Wang Yanan, Kong Lingxin, et al. Sustainable antimony upgrading through multi-zone vacuum distillation: eliminating chemical reagents in 4N purity metal production[J]. Separation and Purification Technology, 2026, 382: 135966. DOI: 10.1016/j.seppur.2025.135966.

[17]

黄占超 . 金属锑真空提纯及高纯锑的制备研究[D]. 昆明: 昆明理工大学, 2003: 23-24.

[18]

Huang Zhanchao . Study on vacuum purification of metallic antimony and preparation of high-purity antimony[D]. Kunming: Kunming University of Science and Technology, 2003: 23-24.

[19]

戴永年, 杨斌 . 有色金属真空冶金[M]. 2版. 北京: 冶金工业出版社, 2009: 34-100.

[20]

Dai Yongnian, Yang Bin . Vacuum metallurgy of nonferrous metals[M]. 2nd ed. Beijing: Metallurgical Industry Press, 2009: 34-100.

[21]

孟朝松 . 贵锑真空气化气-液相平衡与熔体中组元逸散规律的研究[D]. 昆明: 昆明理工大学, 2024: 18-43.

[22]

Meng Chaosong . Study on gas-liquid equilibrium of vacuum gasification of precious antimony and volatilization behavior of components in melt[D]. Kunming: Kunming University of Science and Technology, 2024: 18-43.

[23]

许长一 . 金属锑真空蒸馏与区域熔炼杂质迁移规律研究[D]. 昆明: 昆明理工大学, 2025: 15-37.

[24]

Xu Changyi . Study on impurity migration behavior in vacuum distillation and zone refining of metallic antimony[D]. Kunming: Kunming University of Science and Technology, 2025: 15-37.

[25]

朱富龙, 袁海滨, 杨斌, 等 . 对中真空条件下铝蒸气相变形核及冷凝的研究[J]. 真空科学与技术学报, 2011, 31(2): 163-168.

[26]

Zhu Fulong, Yuan Haibin, Yang Bin, et al. Aluminum vapor nucleation in phase transition and its condensation in medium vacuum[J]. Chinese Journal of Vacuum Science and Technology, 2011, 31(2): 163-168.

[27]

Ghasemi M, Zanolli Z, Stankovski M, et al. Size-and shape-dependent phase diagram of In-Sb nano-alloys[J]. Nanoscale, 2015, 7(41): 17387-17396.

[28]

Dinsdale A T . SGTE data for pure elements[J]. Calphad, 1991, 15(4): 317-425.

[29]

Guo Xinyu, Zhao Yun, Zha Guozheng, et al. Research of the evaporation law of elemental antimony under vacuum[J]. Vacuum, 2022, 200: 110985. DOI: 10.1016/j.vacuum.2022.110985.

基金资助

山东省技术创新引导计划(YDZX2024091)

AI Summary AI Mindmap
PDF (17314KB)

0

访问

0

被引

详细

导航
相关文章

AI思维导图

/

〈 〉